AlZn8MgCu
(AZ8GU)
No food using. |
Mechanical characteristics:
|
Nominal chemical compound % (according to the standard EN 573-1): |
Si
|
Fe
|
Cu
|
Mn
|
Mg
|
Cr
|
Zn
|
Remarks
|
Others
|
Al
|
Each
|
Total
|
0,40
|
0,50
|
1,2-1,9
|
0,50
|
2,1-3,1
|
0,05-0,25
|
7,2-8,4
|
0,25 Zr+Ti
|
0,05
|
0,15
|
Reste
|
|
Specific mechanical characteristics: |
Extruded bars (according to the standard EN 755-2) : |
State |
Sizes
mm |
Rm
(MPa) |
Rp0,2
(MPa) |
A
% mini |
A50
% mini |
Diam |
Plat |
mini |
max |
mini |
max |
|
< 100
100 à 125
125 à 150
150 à 180
|
< 100
100 à 125
125 à 150
150 à 180
|
|
- |
|
|
|
|
|
Top of the page
Extruded tubes (according to the standard EN-755-2): |
State |
Sizes
mm
Thickness of wall
|
Rm
(MPa) |
Rp0,2
(MPa) |
A
% mini |
A50
% mini |
mini |
max |
mini |
max |
T6/T6510/T6511
|
£
30
|
610
|
-
|
530
|
-
|
5
|
4
|
|
Top of the page
Extruded sections (according to the standard EN-755-2): |
State |
Sizes mm
Thickness of wall
|
Rm
(MPa) |
Rp0,2
(MPa) |
A
% mini |
A50
% mini |
mini |
max |
mini |
max |
T6/T6510/T6511 |
£
30
|
610
|
-
|
530
|
-
|
5
|
4
|
|
Top of the page
Drawn bars (according to the standard EN-754-2): |
State |
Sizes
mm |
Rm
(MPa) |
Rp0,2
(MPa) |
A
% mini |
A50
% mini |
Diam
|
mini |
max |
mini |
max |
T6 |
|
|
|
500 |
|
|
|
|
Top of the page
Drawn tubes
(according to the standard EN-754-2): |
State |
Sizes mm
Thickness of wall
|
Rm
(MPa) |
Rp0,2
(MPa) |
A
% mini |
A50
% mini |
mini |
max |
mini |
max |
T6/T6510/T6511
|
£
5
5<e£ 20
|
590
590
|
-
-
|
530
530
|
-
-
|
6
7
|
4
5
|
|
Top of the page |